1. Difficulties in grinding and polishing titanium alloys

Preparing metallographic samples of titanium and its alloys poses greater difficulties compared to steel, primarily due to their low polishing efficiency. Excessive cutting and polishing processes can result in the formation of deformation twins in the α phase, disrupting the analysis of the titanium's microstructure.

For pure titanium, cold inlaying is more suitable than hot pressure inlaying. However, this method may alter the hydrogen content and distribution within pure titanium. Removing scratches and achieving plastic rheology during sample preparation presents significant challenges.

CNC1

 

2. Introduction of metallographic characteristics of titanium and titanium alloys

Titanium and titanium alloys have been commercially used for over 50 years, offering advantages such as low density, excellent strength-to-weight ratio, corrosion resistance, and high mechanical strength. However, their production cost is considerably high.

Similar to iron, titanium undergoes allotropic transformations and can be heat-treated like steel. The stability of the α-phase at low temperatures and the β-phase at high temperatures is influenced by alloying elements.

At room temperature, titanium and its alloys exist in stable phases, including alloy-containing α, α-β, and β phases, with two additional phases known as near-α and near-β.

 

3. Development of titanium alloy polishing technology

In the earlier days, mechanical polishing processes for titanium and its alloys were time-consuming, often involving the use of polishing solutions with etchants in the final steps. Electrolytic polishing methods yielded better results but carried certain risks and also exhibited some chemical polishing effects.

 

During the 1970s and 1980s, traditional mechanical polishing methods were still prevalent for titanium and its alloys. In 1984, Springer and Ahmed introduced a three-step polishing method for these materials.

The process begins with flat grinding, utilizing 320-grit sandpaper with water cooling to remove the damage layer caused by cutting. Next, rough polishing is performed using 9μm metaDI diamond polishing paste on TEXMET polishing cloth with distilled water as a cooling lubricant. Finally, final polishing involves using MICROCLOTH or MASTERTEX polishing cloth with MASTERMET silica suspension polishing liquid.

 

4. Springer and Ahmed titanium alloy three-step polishing technology

Step 1: Flat Grinding

Use 320-grit sandpaper with water cooling for 2-3 minutes to achieve a flat surface.

Apply 320-grit SiC sandpaper with water cooling, rotating at 240RPM, and a pressure of 27N (6lbs) per sample until smooth.

 

Step 2: Rough Polishing

Apply 9μm metaDI diamond polishing liquid and metaDI polishing lubricant on ULTRA-PAD polishing surface.

Polish at a rotation speed of 120RPM in reverse rotation, applying a pressure of 27N (6lbs) per sample for 10 minutes.

 

Step 3: Final Polishing

Use MICROCLOTH or MASTERTEX polishing cloth with MASTERMET silica polishing solution.

Polish at a rotation speed of 120RPM in reverse rotation, applying a pressure of 27N (6lbs) per sample for 10 minutes.

 

Note: During the polishing process, the sample needs to rotate the direction regularly. Hard phase exists in most metal alloys. If the direction is not rotated, the polished sample will have a black "long tail" on the hard phase, which affects the metallographic quality. The key to the "long tail" problem is the direction of turning the sample. You can turn 90 degrees or 180 degrees each time.

CNC2

5. Müller titanium alloy three-step polishing technology

Step 1: P500 Sandpaper Grinding

Use water-cooled P500 sandpaper at a speed of 300RPM and apply a pressure of 16.7N (3.75lb) per sample during the entire preparation time.

 

Step 2: P1200 Sandpaper Grinding

Use water-cooled P1200 sandpaper at a speed of 300RPM, applying a pressure of 16.7N (3.75lb) per sample for 30 seconds.

 

Step 3: Polishing with Synthetic Lint-Free Cloth and Silica Suspension Polishing Solution

Use a polishing machine at a rotation speed of 150RPM.

Apply a pressure of 33N (7.5lb) per sample for 10 minutes, followed by a pressure of 16.7N (3.75lb) per sample for 2 minutes.

 

Finally, apply a pressure of 8N (2lb) per sample for 1 minute.

The polishing agent composition consists of SiO2 (260ml) + H2O2 (40ml, 30% concentration) + HNO3 (1ml) + HF (0.5mL).

 

6. The difference between manual polishing and machine polishing

Manual polishing requires experience, as it involves mastering key parameters such as strength, time, and speed. In contrast, machine polishing only requires setting the parameters. Beginners often face challenges like insufficient polishing or over-polishing due to impatience.

Both manual and machine polishing follow similar principles. However, manual polishing requires patience and repeated efforts to achieve the desired results. It is crucial to carefully summarize experiences and remain persistent, as the rewards will eventually come.